Why Do Tack Welds Crack on Assembled H Beams Before SAW Welding?
Why do tack welds crack on assembled H beams before the SAW pass?
Tack welds crack because three conditions combine: rapid cooling, hydrogen and restraint. A tack is a tiny weld deposited onto a large, cold plate that acts as a heat sink, so the tack quenches far faster than a continuous bead - on thicker or higher-carbon steels this can form brittle martensite. Hydrogen from damp plate, oil, shop-floor humidity or unburned consumables migrates into that hard structure. The short tack is surrounded by rigid cold metal, so shrinkage creates triaxial tensile stress right at the start and stop craters, where hydrogen cracks initiate. Remove any one leg of this triad and cracking stops: preheat the tack area, use dry low-hydrogen consumables, and keep tack size proportionate so restraint stress stays low. On thin mild steel at room temperature the risk is small; on 25 mm+ flanges or Q355 and above, every tack should be treated as a real production weld.
What size and spacing should H beam tack welds be?
Tacks must be long and thin, never short and fat. Standard practice for H beam assembly: tack length around 50 mm (40-80 mm depending on section), spacing no more than 300-500 mm, tack leg size between one-half and two-thirds of the designed fillet leg, and the first tack at least 50 mm away from each beam end. On the YOMI horizontal assembly machine the PLC stores tack length and interval as a recipe per beam size - typically 50-80 mm length at 300-500 mm intervals executed by the tack torches while the beam travels at 150-1500 mm/min - so quality does not depend on the operator judging it by eye. Oversized tacks become embedded in the main SAW weld and cause defects; undersized, closely spaced tacks cannot hold the fit-up against SAW shrinkage.
Can you run the SAW pass over a cracked or porous tack weld?
Never. A crack in a tack continues straight into the production weld, where it is buried, invisible to surface inspection and far more expensive to repair. AWS D1.1 treats tack welds that remain in place as part of the finished weld, so they must meet the same workmanship standard - same qualified welder, same consumables, same preheat as the main weld. If a tack shows cracks, porosity or incomplete fusion, grind it out completely, clean the area, and re-tack before the beam moves to SAW. A quick daily habit on the assembly line: inspect each tack visually as the beam exits (cracks often show as a hairline through the crater), and tap-test suspect tacks. A cracked tack caught at the assembly station costs a minute; caught after SAW and NDT, it costs a weld repair.
How does root gap affect the submerged arc weld downstream?
Root gap is the single biggest fit-up variable for SAW quality. The web must seat tight against the flange face - target 0 to 0.5 mm, ideally zero along the whole joint. Gaps cause burn-through on thinner webs, lack of fusion at the root, porosity as gas escapes through the gap, and inconsistent weld profile that forces the SAW operator to re-tune parameters beam by beam. There is a second, less obvious effect: on a long seam, the SAW process itself pulls the joint - submerged arc joints can open up ahead of the arc if they are under-tacked, so tack spacing must hold the gap the whole length. On the YOMI assembly machine the hydraulic centering cylinders and upper pressure roller press the web down to zero gap before the first tack, which is what lets the downstream SAW parameters stay constant.
Should tack welds be preheated on thick or high-strength flanges?
Yes. If the WPS requires preheat for the production weld, the tack weld needs it too - many shops preheat carefully for the SAW pass but let the tacks go in cold, and the cracked tacks surface weeks later as hydrogen cracks during NDT. As a working rule: flanges below about 20 mm in mild steel at ambient shop temperature can usually be tacked without preheat; Q355 and higher grades, flanges 25 mm and thicker, cold workshops or damp plate should be preheated to the WPS temperature (typically 100-150 degrees C for thicker high-strength sections), and Chinese fabrication practice requires tack preheat to be at least equal to production preheat. Measure with a contact pyrometer or temperature crayon at the tack location, not at the beam end. Preheating a tack adds seconds; repairing a hydrogen crack in a finished beam costs days.
What tack sequence keeps the web from pulling off-center during assembly?
Tack in a balanced sequence so shrinkage forces cancel. Best practice: start at the center of the joint and work outward, alternating between the two flanges; on long seams use a back-step pattern rather than running all tacks end to end. Unbalanced tacking - finishing one side completely before starting the other - accumulates shrinkage in one direction and pulls the web off-center or bows the flange. The four-torch configuration on the YOMI horizontal assembly machine tack welds both sides in the same pass, which naturally balances the shrinkage. Avoid over-tacking: more tacks means more restraint, and excess restraint converts the SAW pass shrinkage into stress that has to go somewhere - usually as flange angular deformation. Use the minimum tack count and spacing that reliably holds fit-up.
Why do tack welds show porosity and spatter on the assembly machine?
Four causes cover almost every case. (1) Contaminated plate - damp, oily or primered steel at the joint: wipe and dry the joint and remove paint at least 20 mm either side of the fillet line. (2) Wrong shielding gas or flow: use CO2 or an 80/20 Ar/CO2 mix at 15-20 L/min, and shield the torch area from workshop drafts and open doors - a gusty tack is a porous tack. (3) Excessive wire stick-out: keep it at 15-20 mm so the arc stays stable. (4) Parameters that do not match the actual root gap or plate thickness. Because the machine executes tack length and spacing from the stored PLC recipe, tune the process rather than blame the operator: weld a test plate of the same thickness and grade, change one variable at a time, and record the winning combination in the recipe for that beam size.
What should you inspect on tack welds before beams go to the SAW station?
A three-part check at the assembly station output. First, tack quality: visual inspection of every tack for cracks, porosity, undercut and undersize - cracked or porous tacks are ground out and re-tacked, never welded over. Second, fit-up geometry: web-to-flange perpendicularity within about 1 mm per 100 mm of flange width (the code limit is b/100), the T-dimension (web centered between flanges) checked at both ends and mid-length, and root gap 0-0.5 mm along the joint. Third, cleanliness: no spatter, moisture or oil in the SAW weld zone, since contaminated edges are the leading cause of SAW porosity. A beam that passes all three checks gives the SAW station a constant joint - which is the real output of a good assembly machine: fit-up geometry so repeatable that downstream welding parameters never need re-tuning.
Technical Specifications of H Beam Horizontal Assembly Machine
| Parameter | Value |
|---|---|
| Share | |
| Categories | H-beam horizontal production line |
| Brand | YOMI CNC Cutting&Welding Machinery |
| Product Specifications | YM-WZL |
| Model | YM-WZL |
| Component material | ≤Q355 |
| Flange width | 140-800mm |
| Flange thickness: | 8-40mm |
| Web Height: | 350-1500mm |
| Web Thickness: | 6-40mm |
| Workpiece length: | 5000-15000mm |
| Conveying speed: | 8700mm/min |
| Welding speed: | 150-1500mm/min |
| Equipment size: | 35m*10m*4m |
Product Gallery







Applications
The H Beam Horizontal Assembly Machine is widely applied in steel structure prefabricated buildings, bridge and infrastructure construction, shipbuilding and marine engineering, heavy machinery manufacturing, power plant and industrial facilities, and offshore wind power structures.
Learn more about the H Beam Horizontal Assembly Machine:
https://www.steelstructurer.com/pid18432013/H-Beam-Horizontal-Assembly-Machine.htm
For more information about H Beam Horizontal Assembly Machine and other steel structure intelligent equipment, contact YOMI CNC Cutting & Welding Machinery. Our team of experts is ready to help you find the best solution for your manufacturing needs.

- Full Name:
- YOMI WhatsAPP
- Tel:
+86 19053498672
- Email:
- sales@yomi-china.com
- WhatsApp:
- 8619053498672
- Address:
- Factory Adress: 9 Changjie Road, Ningjin,Dezhou, P.R.China